P355GH Boiler Zoo Hlau Phaj

Jan 17, 2025 Tso lus

Qhov kub ntawm P355GH yog dab tsi?

TS EN 10028-2 Qib P355GH Siab Vessel Steel Phaj Haum rau 400 ºC Kub.

 

P355GH VS S355J2

P355GH tshuaj muaj pes tsawg leeg

P355GH tshuaj muaj pes tsawg leeg

Qib

Cov ntsiab lus Max (%)

C

Si

Mn

P

S

Al (min)

N

P355GH

0.10-0.22

0.60

1.10-1.70

0.025

0.015

0.020

0.012

Cr

Cu

Mo

Nb

Ni

Ti

V

0.30

0.30

0.08

0.040

0.30

0.03

0.02

 

S355J2 Tshuaj muaj pes tsawg leeg

C

Si

Mn

Ni

P

S

Cr

Mo

max 0.24

0.60

1.70

 

Max 0.035

Max 0.035

 

 

V

Nb

Ti

N

Cu

 

 

 

 

 

 

 

0.60

 

 

 

 

P355GH Mechanical Property

Qib

 

P355GH Mechanical Property

Thickness

Yield

Tensilmie

Elongation

Impact Zog (KV J) min

P355GH

mm

Min Mpa

Mpa

Tsawg%

-20 degree

0 degree

+20 degree

Tsawg dua los yog sib npaug li 16

355

510-650

20

27

34

40

16>mus tsawg dua los yog sib npaug li 40

345

510-650

20

27

34

40

40>kom tsawg dua los yog sib npaug li 60

335

510-650

20

27

34

40

60>kom tsawg dua los yog sib npaug li 100

315

490-630

20

27

34

40

100>los tsawg dua los yog sib npaug li 150

295

480-630

20

27

34

40

150>mus tsawg dua los yog sib npaug li 250

280

470-630

20

27

34

40

S355J2 Mechanical Property

 

-150

150-250

250-400

 

Tsawg zog nominal thicknessTemperature (-20)

27

27

27

 

Nominal thickness (hli)

rau 16

16 - 40

40 - 63

63 - 80

80 - 100

100 - 150

150 - 200

200-250

250-400

ReH - Yam tsawg kawg nkaus tawm lub zog (MPa)

355

345

335

325

315

295

285

275

265

Nominal thickness (hli)

-3

3-100

100-150

150-250

250-400

Rm -Tensile zog (MPa)

510-680

470-630

450-600

450-600

450-600

 

Nominal thickness (hli)

3-40

40-63

63-100

100-150

150-250

250-400

A - Tsawg kawg elongation Lo=5,65 √ Yog li (%)

22

21

20

18

17

17